Aluminium alloys are not difficult because they are hard. They are difficult because they are soft, ductile and have a low melting point. A drill that rubs instead of cutting will weld aluminium to its own flutes within a few hundred holes.
The rule for this material is short. Use a sharp, polished, uncoated or DLC tool, run it fast, and keep the chip moving.
What actually fails first
Three mechanisms account for most micro drill losses in aluminium.
Built-up edge. Pressure and temperature at the rake face let work material weld to the edge. The edge grows a lump of aluminium, which cuts an oversized, rough hole. When the lump breaks away it takes carbide with it.
Chip packing. Aluminium chips are soft and do not break. In a hole deeper than 3 x D they compact in the flutes and torque climbs until the tool twists off.
Adhesion on the margin. Aluminium smears along the margin, which raises friction and heat. This is where a polished flute earns its cost.
Abrasion is not on the list. Aluminium contains little that wears carbide, so coating hardness is not the deciding factor here.
Coating: uncoated or DLC
Uncoated carbide, polished, is the default. The edge can be ground to a smaller radius, and there is no coating thickness to blunt a 0.1 mm drill.
DLC is the alternative. Its friction coefficient against aluminium is low, and that is what stops the smearing. The limit is temperature: DLC starts to degrade above roughly 350-400 °C. Run it dry at high speed and the layer graphitises.
TiN is the wrong choice. Aluminium adheres to TiN readily, so the built-up edge returns. TiN also needs temperatures that aluminium cannot carry away from the edge.
| Coating | Hardness | Service limit | Verdict for aluminium |
|---|---|---|---|
| Uncoated | 1800-2000 HV | edge-limited | Default: sharpest edge, lowest cost |
| DLC | 1800-2200 HV | 350-400 °C | Gummy alloys, needs cooling |
| TiN | 2400-2500 HV | 550-600 °C | Not recommended: adhesion |
Geometry
118° is the standard point for aluminium. It works, provided the chisel edge is thinned. A heavy web in soft material means high thrust at the point where the drill is weakest.
Two flutes with a high helix clear soft chips better than a low helix. In practice, a polished flute matters more than the helix angle.
Starting parameters
For a 1.0 mm drill in wrought alloy:
- Cutting speed 150-250 m/min. That is 48,000-80,000 rpm at 1.0 mm, above most micro spindles. The spindle limit is acceptable.
- Feed per revolution 0.005-0.02 mm, scaled with diameter. Under-feeding is the common error: it converts cutting into rubbing.
- Peck every 2-3 x D to clear chips, even with through-coolant.
The diameter relationship is worth stating once:
n = 1000 x vc / (pi x D)
At vc = 200 m/min and D = 0.5 mm this gives 127,000 rpm, which no micro spindle reaches. Run at maximum spindle speed and accept the lower effective speed.
Series that fit this job
DC326 is the uncoated general series: 0.04-3.175 mm, 542 part numbers, ground to -0.003 mm on the standard record.
DC336 is the DLC series, 0.07-4.98 mm, for gummy alloys and longer runs.
EC326 covers flat-bottom end mills up to 16 mm when the operation is a slot rather than a hole.
FAQ
Do I need coolant for a 0.5 mm hole in aluminium?
MQL is enough up to about 3 x D. Beyond that, use through-tool coolant or peck with an air blast. Flood coolant works but rarely reaches the bottom of a deep micro hole.
Why is my hole oversized?
Almost always built-up edge or runout. Check runout first: above 0.005 mm at 0.5 mm diameter the drill acts as a single-flute cutter. If runout is fine, the coating is wrong or the speed is too low.
Can I drill aluminium with a TiN drill in an emergency?
Yes, at reduced speed, and expect a short life. Clean the flutes after every few holes.